a me Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012-10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton b1H Test Date: __:1.:.,:/2:..:6.:.,:/2:...:0....:.14-=------,--------L'phi/tlf Reviewed By: Allen Cottingham 1
f{\\W..
Review Date: 1/30/2014 1..00 -' 1~
Rock Type Moisture Condition Specimen Diameter, (in)
Specimen Length, (in)
Length/Diameter Ratio Sample No.: L3-29 BH Boring No.: MP-118 Run. No.: N/A Sample Depth (ft): 97.6-99.0 Page 1 of 2 (See boring log)
Laboratory Air-Dry 2.39 5.33 2.2 Yes Specimen Conforms with Dimensional Requirements?
As-Tested Unit Weight, (pcf)
'46&:t" I "~ H.> ~
~
b 1/)
~
- 5,000
-4,500
-4,000
- 3,500
- 3,000
- 2.500
- 2.000
- 1,500
-1,000
- 500 0
0.0020 Comments:
Loading Rate {lb/sec) 160 v
Test Duration to Failure, (min) 4.7 Uniaxial Compressive Strength, (psi) 4,870 Type of Break Shear Young's Modulus, (psi) 2,490,000 Poisson's Ratio 0.20 l
I
~
I I I I
I I
\\
I I
I I
I
\\
I I
I I
\\
I /
I 1-I I
/
I I
/
Average Adjusted Axial i
I 0.0010 0.0000 l aterilt Strain ( + ),(in/In}
/
.().0010 Strain (in/in)
Average Adjusted Lateral Strain (infln)
.().0020 Axial Strain I * ), (In/In)
Young's Modulus and Poisson's Ratio determined using linear least-squares of stress-strain data from 40% to 60%
of the uniaxial compressive strength (data points used are indicated on the figure above).
Axial Strain is negative; Lateral Strain is positive.
Load direction with respect to lithology: Vertical Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-20 of 91 1
r
- 0.0030
a me Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012-10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton 1r1 Test Date: 1/26/2014
~N Reviewed By: Allen Cottingham f'\\~
Review Date:...:1.:.:/3:..:0.:..:/2:.:0...:.1..:.4 ______ 1.)0-ll/
Comments:
Specimen Prior to Testing
("MP-118 LJ-29 BH before test.jpg"):
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-21 of 91 Sample No.: LJ-29 BH Boring No.: MP-11 B Run. No.: N/A Sample Depth (ft): 97.6-99.0 Page 2 of 2 Specimen After Testing
("MP-118 LJ-29 BH after test.jpg"):
a me Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012*10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton ltlH Test Date:....:1:..::/2:..::6/c::2:..::01.:....4:..__ ___
....t,£f.-JI BI/ Jlf Reviewed By: Allen Cottingham l"\\Pl.
Review Date: 1/30/2014 1-;H4 Rock Type Moisture Condition Specimen Diameter, (in)
Specimen Length, (In)
Length/Diameter Ratio Specimen Conforms with Dimensional Requirements?
Sample No.: L3-31 BCH Boring No.: MP-122 Run. No.: N/A Sample Depth (ft): 144.3-145.1 Page 1 of 2 (See boring log)
Laboratory Air-Dry 2.40 5.10 2.1 Nol1>
As-Tested Unit Weight, (pcf) 4%:6-I r,q f/et; Loading Rate (lb/sec) 160 v
Test Duration to Failure, (min) 6 Uniaxial Compressive Strength, (psi) 12,430 Type of Break Columnar Young's Modulus, (psi) 5,550,000 Poisson's Ratio 0.22
-14,000
- 12,000
- 10,000
-8,000
.e
-6,000 (I)..
~
-4,000
- 2,000
--Average Adjusted Axial Strain (in/in) l
--Average Adjusted Lateral Strain (in/in) J 0
0.0020 0.0010 Lateral Strain I * ], (In/In)
Comments:
0.0000
.0.0010
- 0.0020 Axial Strain ( *],(In/In)
Young's Modulus and Poisson's Ralio determined using linear least-squares of slress-strain data from 40% to 60%
of the uniaxial compressive slrenglh (data points used are indicated on the figure above).
Axial Strain is negative; Lateral Strain is positive.
Load direction with respect to lithology: Vertical (l ) Specimen did not meet End Flatness requirements of ASTM 04543-08. Authorization to proceed with test received from John Damm.
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-22 of 91
- 0.0030
a me Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012-10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton IJI H Test Date:...:1.:..:/2:..:.6:.::/2:..:.0-'-14'--____
...~./+-'
/ ~t/N Reviewed By: Allen Cottingham r
.>J~Fr{,
Review Date: 1/30/2014 1 -)o-t1 Comments:
Specimen Prior to Testing
("MP-122 L3-31 BCH before test.jpg"):
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-23 of 91 Sample No.: L3-31 BCH Boring No.: MP-122 Run. No.: N/A Sample Depth (ft): 144.3-145.1 Page 2 of 2 Specimen After Testing
("MP-122 L3-31 BCH after test.jpg"):
Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 0 7012*1 0 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton mrit Test Date: _1,;...,/7_;_/2-'0_1_4 ______ 1/t:z/*'-1 Reviewed By: Allen Cottingham f"(!rC Review Date: 1/21/2014 t* 1A
- 1't Rock Type Moisture Condition Specimen Diameter, (in)
Specimen Length, (in)
Length/Diameter Ratio Specimen Conforms with Dimensional Requirements?
As-Tested Unit Weight, (pcf) loading Rate (lb/sec)
Test Duration to Failure, (min)
Uniaxial Compressive Strength, (psi)
Type of Break Young's Modulus, (psi)
Poisson's Ratio
- 6.000 I
Sample No.: L2-13-BCH Boring No.: MP-201 Run. No.: N/A Sample Depth (ft): 130.6'*131.8' Page 1 of 2 (See boring log)
Laboratory Air-Dry 2.39 5.67 2.4 No 111
~
(G. f) l)eJ, 130
~
4 5,000 shear 11,080,000 0.29 t,(A-f¥4
- 5.000
" t
~
-4,000
- 3.000
(
/
I I
f
- 2,000 ----
-~---
-1.000
-\\1 I
-- Average Adjusted Axial,__
I I
i Strain (in/in) 0 0.0020 Comments:
0.0010 0.0000 Lateral Strain I +], (In/in)
-0.0010
-- Average Adjusted l ateral Strain (in/in)
-ll.0020 Alllal Strain I *), (In/In)
- 0.0030 Young's Modulus and Poisson's Ratio determined using linear least-squares of stress-strain data from 40% to 60%
of the uniaxial compressive strength (data points used are indicated on the figure above).
Axial Strain is negative; Lateral Strain is positive.
Load direction with respect to lithology: Vertical (II Specimen did not meet end purpendicularity, end parrallelism and end flatness requirements of ASTM 04543-08. Authorization to proceed with test received from John Damm.
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-24 of 91
a me Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012-10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton tntr'A Test Date: 1/7/2014 1/1.-'t /N
~~~-----------
Reviewed By: Allen Cottingham
.~
Review Date: 1/21/2014 1, -z.,l
- t~
Specimen Prior to Testing
("MP-201 L2-13 BCH before test.jpg")
Comments:
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-25 of 91 Sample No.: L2-13-BCH Boring No.: MP-201 Run. No.: N/A Sample Depth (ft): 130.6'-131.8' Page 2 of2 Specimen After Testing
("MP-201 L2-13 BCH after test (2).jpg"):
a me Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012-10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton
~~;4 Test Date: -'1-':-'/7.;..:/2:;.;;0-,:.14..:......, _____ t/t1/l ~
Reviewed By: Allen Cottingham lfi/'It.
Review Date: 1/21/2014
,.,,. t~
Rock Type Moisture Condition Specimen Diameter, (in)
Specimen Length, (in)
Length/Diameter Ratio Sample No.: L2-14-BCH Boring No.: MP-201 Run. No.: NIA Sample Depth (ft): 186.2'-186.6' Page 1 of 2 (See boring log)
Laboratory Air-Dry 2.39 4.93 2.1 Specimen Conforms with Dimensional Requirements?
No()
As-Tested Unit Weight, (pcf)
Loading Rate (lblsec)
Test Duration to Failure, (min)
Uniaxial Compressive Strength, (psi)
Type of Break Young's Modulus, (psi)
Poisson's Ratio
- 10,000
.a.ooo 1 ---~-
...e
-6,000
~
Cl)
~
-4,000
- 2,000 -
~t ~ ef!eCJ.
130 v
8 9,900 shear 3,700,000 0.22
--Average Adjusted Axial
'-'-----~
Strain {in/in)
--Average Adjusted Lateral Strain {in/in) 0 ~------------~-------'------------------------------------------~
0.0010 0.0005 0.0000
.().0005
.().0010
.().0015
.Q.0020
.().0025
.().0030
.().0035
-0.0040 Lateral Stroln ( + ], (lnfln)
Axial Strain ( -], (In/in)
Comments:
Young's Modulus and Poisson's Ralio determined using linear least-squares of stress-strain data from 40% to 60%
of the uniaxial compressive strength {data points used are indicated on the figure above).
Ax*al Strain is negative; Lateral Strain is positive.
Load direction with respect to lithology: Vertical 1'1 Specimen did not meet side straightness, end purpendicularity, end parrallelism, and end flatness requirements of ASTM 04543-08. Authorization to proceed with test received from John Damm.
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-26 of 91
Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012-10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton
/hli tJ Test Date:...:;1n:.:.../:.=2.::...01:...:4 ____
t/1'1/14 Reviewed By: Allen Cottingham rll4t:
Review Date: 1/21/2014 1-J,l-lq Comments:
Specimen Prior to Testing
("MP-201 L2-14 BCH before test.jpg"):
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-27 of 91 Sample No.: L2*14-BCH Boring No.: MP-201 Run. No.: N/A Sample Depth (ft): 186.2'-186.6' Page 2 of2 Specimen After Testing
("MP-201 L2-14 BCH after test (2).jpg"):
a me Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012-10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton M,;;J Test Date: _1'"'/7...:.;/2.;.;;0..;.14~----- 'ftt/lli Reviewed By: Allen Cottingham
.M,f({.
Review Date: 1/21/2014 j-'2.1-\\.Aj Rock Type Moisture Condition Specimen Diameter, (in)
Specimen Length, (in)
Length/Diameter Ratio Specimen Conforms with Dimensional Requirements?
As-Tested Unit Weight, (pcf)
Loading Rate (lb/sec)
Test Duration to Failure, (min)
Uniaxial Compressive Strength, (psi)
Type of Break Young's Modulus, (psi)
Poisson's Ratio Sample No.: L2*16-BH Boring No.: MP-201 Run. No.: N/A Sample Depth (ft): 338.3'-339.7' Page 1 of 2 (See boring Jog)
Laboratory Air-Dry 2.40 5.24 2.2 No 11l
~
t 1.> JtY.).
130 v
13.7 21,910 Columnar 12,840,000 0.30
~/14
- 25.000,..-------------------------------------,
.e..
R
'i'l
~
-20,000
- 15,000
- 10,000
-5,000
- Average Adjusted Axial Strain (in/in)
--Average Adjusted Lateral Strain (in/in) oL-______________ r~------------------~====~__J 0.0010 0.0005 0.0000
-0.0005
~.0010
-0.0015
~.0020 Lateral Strain I+ 1. (In/in)
Axial Strain I -1. (In/In)
Comments:
Young's Modulus and Poisson's Ratio determined using linear least-squares of stress-strain data from 40% to 60%
of the uniaxial compressive strength (data points used are indicated on the figure above).
Axial Strain is negative; Lateral Strain is positive.
Load direction with respect to lithology: Vertical
<*l Specimen did not meet end purpendicularily requirements of ASTM D4543-08.
Authorization to proceed with lest received from John Damm.
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-28 of 91
a me Elastic Moduli of Intact Rock Core Specimens in Uniaxial Compression ASTM 07012-10 Project Name: Clinch River SMR Project Number: 6468-13-1072 Tested By: Mike Hamilton r19tt Test Date:_1.:../7"'"'/2_0_14 ______ ",ltt(l'f Reviewed By: Allen Cottingham
",(\\<.
Review Date: 1/21/2014 1-l.l-1 ~
Comments:
Specimen Prior to Testing
("MP-201 L2-16 BH before test.jpg"):
Clinch River Data Report Rev. 4 CRP-1112.16 Page G.2-29 of 91 Sample No.: L2-16-BH Boring No.: MP-201 Run. No.: N/A Sample Depth (ft): 338.3'-339.7' Page 2 of2 Specimen After Testing
("MP-201 L2-16 BH after test (2).jpg"):